For the purpose of this Subsection, the definitions given in accepted standards [6-5A(2)] shall apply.
1.1 This Code (Part 6/Subsection 5A) deals with the general structural use of plain and reinforced concrete.
1.1.1 For the purpose of this Subsection, plain concrete structures are those where reinforcement, if provided is ignored for determination of strength of the structure.
1.2 Special requirements of structures, such as shells, folded plates, arches, chimneys, blast resistant structures, hydraulic structures, liquid retaining structures and earthquake resistant structures, covered in respective Indian Standards, have not been covered in this Subsection; these Indian Standards shall be used in conjunction with this Subsection. See good practices [6-5A(1)].
This Code (Part 6/Subsection 5A) covers the structural design aspects of plain and reinforced concrete.
The Section 5 of Part 6 of the Code covers plain and reinforced concrete and also the prestressed concrete. The Section has been subdivided into the following subsections:
5A Plain and Reinforced Concrete
5B Prestressed Concrete
This Subsection 5A was first published in 1970 as Subsection 5A of SP 7 (Part 6) and was subsequently revised in 1983 and 2005, to bring it in line with revised version of IS 456 : 1978 and IS 456 : 2000, respectively on which this chapter was based.
The second revision (NBC 2005) incorporated a number of important changes. The major thrust being:
a) In recent years, durability of concrete structures have become the cause of concern to all concrete technologists. This has led to codify the durability requirements world over. In this revision of the Code, in order to introduce in-built protection from factors affecting a structure, earlier clause on durability has been elaborated and a detailed clause covering different aspects of design of durable structure has been incorporated.
b) Sampling and acceptance criteria for concrete have been revised. With this revision acceptance criteria has been simplified in line with the provisions given in BS 5328 (Part 4): 1990 'Concrete: Part 4 Specification for the procedures to be used in sampling, testing and assessing compliance of concrete'.
Some of the significant changes incorporated in the 2005 version were: inclusion of all the three grades of ordinary Portland cement, namely 33 Grade, 43 Grade and 53 Grade and sulphate resisting Portland cement in the list of types of cement used (in addition to other types of cement); modification of the permissible limits for solids in water keeping in view the durability requirements; modification of the clause on admixtures in view of the availability of new types of admixtures including superplasticizers; inclusion of grades higher than M 40 in Table 2 'Grades of Concrete'; recommendations regarding minimum grade of concrete to be not less than M 20 in reinforced concrete work (see also 5.1.3); revision of the formula for estimation of modulus of elasticity of concrete; specification of workability only in terms of slump, in the absence of proper correlation between compacting factor, vee-bee time and slump, modification of the clause on 'Durability' to include detailed guidance concerning the factors affecting durability; modification of the table on 'Environmental Exposure Conditions' to include 'very severe' and 'extreme' exposure conditions, also covering requirements for shape and size of member, depth of concrete cover, concrete quality, requirement against exposure to aggressive chemical and sulphate attack, minimum cement requirement and maximum water cement ratio, limits of chloride content, alkali silica reaction, and importance of compaction, finishing and curing; incorporation of a clause on 'Quality Assurance Measures' to give due emphasis to good practices of concreting; introduction of proper limits on the accuracy of measuring equipments to ensure accurate batching of concrete; modification of the clause on 'Construction Joints'; and modification of the clause on 'Inspection' to give more emphasis on quality assurance.
The significant changes incorporated in Section 5A (C) of the 2005 version were: detailing of requirements for ‘Fire Resistance’; modification of the figure for estimation of modification factor for tension reinforcement used in calculation of basic values of span to effective depth to control the deflection of flexural member; addition of recommendations regarding effective length of cantilever; addition of recommendations regarding deflection due to lateral loads; inclusion of recommendations for adjustments of support moments in restrained slabs; introduction of stability index in the determination of effective length of compression members, to determine sway or no sway conditions; inclusion of recommendations for lap length of hooks for bars in direct tension and flexural tension; modification of recommendations regarding strength of welds; modification in recommendations regarding cover to reinforcement; prescription of cover based on durability requirements for different exposure conditions; introduction of the term ‘nominal cover’; and prescription of the cover based on durability requirement as well as for fire requirements.
The significant change incorporated in Section 5A (D) of the 2005 version included modification of the clause on walls. The modified clause includes design of walls against horizontal shear.
In Section 5 of the 2005 version on limit state method, a new clause was added for calculation of enhanced shear strength of sections close to supports. Some modifications were also made in the clause on Torsion. Formula for calculation of crack width were added (separately in Annex F).
Working stress method was added in Annex A so as to give greater emphasis to limit state design. In this annex, modifications regarding torsion and enhanced shear strength on the same lines as in Section 5 have been made.
Whilst the common methods of design and construction have been covered in this code, special systems of design and construction of any plain or reinforced concrete structure not covered by this code may be permitted on production of satisfactory evidence regarding their adequacy and safety by analysis or test or both (see 18).
In this Code it has been assumed that the design of plain and reinforced cement concrete work is entrusted to a qualified engineer and that the execution of cement concrete work is carried out under the direction of a qualified and experience supervisor.
In this third revision of this Subsection, the following major modifications have been incorporated:
a) All the 4 amendments so far issued to IS 456 : 2000 ‘Code of practice for plain and reinforced concrete (fourth revision)’ have been incorporated.
b) Provisions relating to use of mineral admixtures, their effects on properties of fresh and hardened concrete have been elaborated, including precautions associated therewith.
c) Aggregates from other than natural sources, including iron slag aggregate, steel slag aggregate, copper slag aggregate, bottom ash from thermal power plant, and aggregate derived from construction and demolition waste, have been included through cross reference to the revised IS 383, namely IS 383 : 2016 ‘Specification for coarse and fine aggregate for concrete (third revision)’.
d) Provisions relating to stripping time of forms for beams and slabs have been modified, also emphasizing the need for immediate replacement of props have been included.
e) The stripping time in case of the concrete made using cement other than OPC or using cementitious materials like fly ash and slag, has been specified, also giving guidance on minimum cube strength requirements of concrete before removal of formwork in case provision of stripping time applicable for concrete made using OPC, is to be used.
f) Provisions related to self compacting concrete (SCC) and high performance concrete (HPC) have been included as part of special concretes.
g) Design provisions related to steel fibre reinforced concrete have been included as part of special concretes.
h) Provisions related to shear stress for coupled shear walls have been included.
j) Comprehensive provisions on ductile detailing have been included from IS 13920 : 2016 ‘Code of practice for ductile detailing of reinforced concrete structures subjected to seismic forces (first revision)’ to help extensive implementation of ductile detailing provisions in all relevant structures.
k) List of Indian Standards referred as good practice has been updated, especially in view of formulation of a number of new/revision of Indian Standards relating to concrete.
This Subsection is largely based on the following Indian Standards:
IS 456 : 2000 Code of practice for plain and reinforced concrete (fourth revision)
IS 13920 : 2016 Code of practice for ductile detailing of reinforced concrete structures subjected to seismic forces (first revision)
All standards, whether given herein above or cross-referred to in the main text of this Subsection, are subject to revision. The parties to agreement based on this Subsection are encouraged to investigate the possibility of applying the most recent editions of the standards.
For the purpose of deciding whether a particular requirement of this Subsection is complied with, the final value, observed or calculated, expressing the result of a test or analysis, shall be rounded off in accordance with IS 2 : 1960 ‘Rules for rounding off numerical values (revised)’. The number of significant places retained in the rounded off value should be the same as that of the specified value in this Subsection.
(a) General
For the purpose of this Subsection, the following letter symbols shall have the meaning indicated against each; where other symbols are used, they are explained at the appropriate place:
A — Area
b — Breadth of beam, or shorter dimension of
a rectangular column
bef — Effective width of slab
bf — Effective width of flange
bw — Breadth of web or rib
D — Overall depth of beam or slab or diameter of column; dimension of a rectangular column in the direction under consideration
Df — Thickness of flange
DL — Dead load
d — Effective depth of beam or slab
d' — Depth of compression reinforcement from the highly compressed face
Ec — Modulus of elasticity of concrete
EL — Earthquake load
Es — Modulus of elasticity of steel
e — Eccentricity
s — Spacing of stirrups or standard deviation
w
wd — Distributed dead load per unit area
w₁ — Distributed imposed load per unit area
γf
γm
δm — Percentage reduction in moment
σcbc — Permissible stress in concrete in bending compression
σcc — Permissible stress in concrete in direct compression
σmc — Permissible stress in metal in direct compression
σsc — Permissible stress in steel in compression
σst — Permissible stress in steel in tension
σsv — Permissible stress in shear reinforcement
τbd — Design bond stress
τc — Shear stress in concrete
τc, — Maximum shear stress in concrete with shear reinforcement
τv — Nominal shear stress
— Diameter of bar
The cement used shall be any of the following conforming to accepted standards [6-5A(3)] and the type selected should be appropriate for the intended use:
a) Ordinary Portland cement,
b) Rapid-hardening Portland cement,
c) Portland slag cement,
d) Portland pozzolana cement (fly ash based),
e) Portland pozzolana cement (calcined clay based),
f) Hydrophobic cement,
g) Low heat Portland cement, and
h) Sulphate resisting Portland cement.
Other combinations of Portland cement with mineral admixture (see 4.2) of quality conforming with relevant Indian Standards laid down may also be used in the manufacture of concrete provided that there are satisfactory data on their suitability, such as performance test on concrete containing them.
4.1.1 Low heat Portland cement conforming to accepted standards [6-5A(4)] shall be used with adequate precautions with regard to removal of formwork, etc.
4.1.2 High alumina cement conforming to accepted standard [6-5A(5)] or supersulphated cement conforming to accepted standard [6-5A(6)] may be used only under special circumstances with the prior approval of the Engineer-in-Charge. Specialist literature may be consulted for guidance regarding the use of these types of cements.
4.1.3 The attention of the Engineer-in-Charge and users of cement is drawn to the fact that quality of various cements mentioned in 4.1 is to be determined on the basis of its conformity to the performance characteristics given in the respective Indian Standard specification for that cement. Any trade-mark or any trade name indicating any special features not covered in the standard or any qualification or other special performance characteristics sometimes claimed/indicated on the bags or containers or in advertisements alongside the ‘Statutory Quality Marking’ or otherwise have no relation whatsoever with the characteristics guaranteed by the Quality Marking as relevant to that cement. Consumers are, therefore, advised to go by the characteristics as given in the corresponding Indian Standard Specification or seek specialist advice to avoid any problem in concrete making and construction.
Mineral admixtures listed below may be used along with ordinary Portland cement. Uniform blending of the additions with the cement should be ensured. For this purpose, specific facility is required to be available at the construction site or RMC plant.
NOTE — In case more than one type of mineral admixture is to be used in the same concrete or mineral admixture is used along with blended cement, the necessary trials for suitability of concrete so made shall be done and duly approved by the Engineer-in-Charge.
Pozzolanic materials as given below may be used.
Fly ash conforming to accepted standard [6-5A(7)] may be used as part replacement of ordinary Portland cement.
Silica fume conforming to accepted standard [6-5A(8)] may be used as part replacement of ordinary Portland cement. Silica fume is usually used in proportion of 5 to 10 percent of the cement.
Rice husk ash giving required performance and uniformity characteristics may be used with the approval of the Engineer-in-Charge.
NOTE — Rice husk ash is produced by burning rice husk and contains large proportion of silica. To achieve amorphous state, rice husk may be burnt at controlled temperature. It is necessary to evaluate the product from a particular source for performance and uniformity since it can be as deleterious as silt when incorporated in concrete. Water demand and drying shrinkage should be studied before using rice husk.
Metakaolin conforming to accepted standard [6-5A(9)] may be used as part replacement of ordinary Portland cement.
Ground granulated blast furnace slag obtained by grinding granulated blast furnace slag conforming to accepted standards [6-5A(10)] may be used as part replacement of ordinary Portland cement.
4.2.3.1 For concrete made with mineral admixtures, the setting time and rate of gain of strength may be different from those of concrete made with ordinary Portland cement alone. Cognizance of such modified properties shall be taken into account in deciding de-shuttering time, rate of movement of formwork in slipform construction, initial time of prestressing, longer curing period and for early age loading. The compatibility of chemical admixtures and cementitious materials should be ensured by trials.
Concrete containing mineral admixtures generally have equal or improved finishability compared to similar concrete mixes without them. Mixes that contain high dosages of mineral admixtures, specially silica fume, can be sticky and difficult to finish.
Concrete containing mineral admixtures may exhibit an increase in plastic shrinkage cracking because of its low bleeding characteristics. The problem may be avoided by ensuring that such concrete is protected against drying, both during and after finishing.
4.2.3.2 Compatibility of chemical admixtures and superplasticizers conforming to accepted standards [6-5A(11)] with the binder system shall be ensured by trials.
4.2.3.3 Some other properties of concrete such as modulus of elasticity, tensile strength, creep and shrinkage are not likely to be significantly different. For design purposes, it will be sufficiently accurate to adopt the same values as those used for concrete made with ordinary Portland cement alone.
Aggregates, derived from natural sources and from other than natural sources, shall comply with the requirements of accepted standards [6-5A(12)].
4.3.1 Other types of aggregates such as crushed overburnt brick or tile, which may be found suitable with regard to strength, durability of concrete and freedom from harmful effects may be used for plain concrete members, but such aggregates should not contain more than 0.5 percent of sulphates as SO₃ and should not absorb more than 10 percent of their own mass of water.
4.3.2 Heavy weight aggregates or light weight aggregates such as bloated clay aggregates and sintered fly ash aggregates may also be used provided the Engineer-in-Charge is satisfied with the data on the properties of concrete made with them.
NOTE — Some of the provisions of the code would require modification when these aggregates are used; specialist literature may be consulted for guidance.
The nominal maximum size of coarse aggregate should be as large as possible within the limits specified but in no case greater than one-fourth of the minimum thickness of the member, provided that the concrete can be placed without difficulty so as to surround all reinforcement thoroughly and fill the corners of the form. For most work, 20 mm aggregate is suitable. Where there is no restriction to the flow of concrete into sections, 40 mm or larger size may be permitted. In concrete elements with thin sections, closely spaced reinforcement or small cover, consideration should be given to the use of 10 mm nominal maximum size.
Plums above 160 mm and up to any reasonable size may be used in plain concrete work up to a maximum limit of 20 percent by volume of concrete when specifically permitted by the Engineer-in-Charge. The plums shall be distributed evenly and shall be not closer than 150 mm from the surface.
4.3.3.1 For heavily reinforced concrete members as in the case of ribs of main beams, the nominal maximum
size of the aggregate should usually be restricted to 5 mm less than the minimum clear distance between the main bars or 5 mm less than the minimum cover to the reinforcement whichever is smaller.
4.3.4 Coarse and fine aggregate shall be batched separately.
Water, natural or treated, used for mixing and curing shall be clean and free from injurious amounts of oils, acids, alkalis, salts, sugar, organic materials or other substances that may be deleterious to concrete or steel.
Potable water is generally considered satisfactory for mixing concrete. As a guide the following concentrations represent the maximum permissible values:
a) To neutralize 100 ml sample of water, using phenolphthalein as an indicator, it should not require more than 5 ml of 0.02 normal NaOH. The details of test are given in 7.1 of good practice [6-5A(13)].
b) To neutralize 100 ml sample of water, using mixed indicator, it should not require more than 25 ml of 0.02 normal H₂SO₄ . The details of test shall be as given in 7 of good practice [6-5A(13)].
c) Permissible limits for solids shall be as given in Table 1.
| Sl No. | Parameter | Tested as Per | Permissible Limit Max |
|---|---|---|---|
| (1) | (2) | (3) | (4) |
| i) | Organic | Good practice [6-5A(13)] | 200 mg/l |
| ii) | Inorganic | Good practice [6-5A(13)] | 3 000 mg/l |
| iii) | Sulphates (as SO3) | Good practice [6-5A(13)] | 400 mg/l |
| iv) | Chlorides (as Cl) | Good practice [6-5A(13)] | 2 000 mg/l for concrete not containing embedded steel and 500 mg/l for reinforced concrete work |
| v) | Suspended matter | Good practice [6-5A(13)] | 2 000 mg/l |
4.4.1 In case of doubt regarding development of strength, the suitability of water for making concrete shall be ascertained by the compressive strength and initial setting time tests specified in 4.4.1.2 and 4.4.1.3.
4.4.1.1 The sample of water taken for testing shall represent the water proposed to be used for concreting,
due account being paid to seasonal variation. The sample shall not receive any treatment before testing other than that envisaged in the regular supply of water proposed for use in concrete. The sample shall be stored in a clean container previously rinsed out with similar water.
4.4.1.2 Average 28 days compressive strength of at least three 150 mm concrete cubes prepared with water proposed to be used shall not be less than 90 percent of the average of strength of three similar concrete cubes prepared with distilled water. The cubes shall be prepared, cured and tested in accordance with good practice [6-5A(14)].
4.5.1 Admixture, if used shall comply with accepted standards [6-5A(15)] . Previous experience with and data on such materials should be considered in relation to the likely standards of supervision and workmanship to the work being specified.
4.5.2 Admixtures should not impair durability of concrete nor combine with the constituent to form harmful compounds nor increase the risk of corrosion of reinforcement.
4.5.3 The workability, compressive strength and the slump loss of concrete with and without the use of admixtures shall be established during the trial mixes before use of admixtures.
4.5.4 The relative density of liquid admixtures shall be checked for each drum containing admixtures and compared with the specified value before acceptance.
4.5.5 The chloride content of admixtures shall be independently tested for each batch before acceptance.
4.5.6 If two or more admixtures are used simultaneously in the same concrete mix, data should be obtained to assess their interaction and to ensure their compatibility.
4.5.7 The amount of admixture added to a mix shall be recorded in the production record. Redosing of admixtures is not normally permitted. In special circumstances, if necessary, additional dose of admixture may be added at project site and mixed adequately in mixer itself to regain the workability of concrete with the mutual agreement between the producer/supplier and the purchaser/user of concrete. However, the producer/supplier shall assure the ultimate quality of concrete supplied by him and maintain record of quantity and time of addition.
The reinforcement shall be any of the following conforming to the accepted standards [6-5A(16)]:
a) Mild steel and medium tensile steel bars.
b) High strength deformed steel bars.
c) Hard-drawn steel wire fabric.
d) Structural steel of Grade A.
4.6.1 All reinforcement shall be free from loose mill scales, loose rust and coats of paints, oil, mud or any other substances which may destroy or reduce bond. Sand blasting or other treatment is recommended to clean reinforcement.
4.6.2 Special precautions like coating of reinforcement may be required for reinforced concrete elements in exceptional cases and for rehabilitation of structures. Specialist literature may be referred to in such cases. Reduction in design bond strength of coated bars shall be looked into.
4.6.3 The modulus of elasticity of steel shall be taken as 200 kN/mm² . The characteristic yield strength of different steel shall be assumed as the minimum yield stress/0.2 percent proof stress specified in the relevant Indian Standard.
Fibres may be added to concrete for special applications to enhance properties, for which specialist literature may be referred to. See also 16B.
Storage of materials shall be as described in good practice [6-5A(17)].
The concrete shall be in grades designated as per Table 2.
| Table 2 Grades of Concrete(Clauses 5.1, 8.2.2, 14.1.1 and 35.1) | |||
| Sl No. | Group | Grade Designation | Specified Characteristic Compressive Strength of 150 mm Cube at 28 Days N/mm² |
| (1) | (2) | (3) | (4) |
| i) | Ordinary concrete | M 10 | 10 |
| M 15 | 15 | ||
| M 20 | 20 | ||
| ii) | Standard concrete | M 25 | 25 |
| M 30 | 30 | ||
| M 35 | 35 | ||
| M 40 | 40 | ||
| M 45 | 45 | ||
| M 50 | 50 | ||
| M 55 | 55 | ||
| M 60 | 60 | ||
| iii) | High strength concrete | M 65 | 65 |
| M 70 | 70 | ||
| M 75 | 75 | ||
| M 80 | 80 | ||
| M 90 | 90 | ||
| M 95 | 95 | ||
| M 100 | 100 | ||
| NOTES1 In the designation of concrete mix, M refers to the mix and the number to the specified compressive strength of 150 mm size cube at 28 days, expressed in N/mm² .2 For concrete of grades above M 60, design parameters given in the standard may not be applicable and the values may be obtained from specialized literatures and experimental results. | |||
5.1.1 The characteristic strength is defined as the strength of material below which not more than 5 percent of the test results are expected to fall.
5.1.2 The minimum grade of concrete for plain and reinforced concrete shall be as per Table 5.
5.1.3 Concrete of grades lower than those given in Table 5 may be used for lean concrete, foundation for masonry walls or temporary reinforced concrete construction.
There is normally a gain of strength beyond 28 days.
The quantum of increase depends upon the grade and type of cement, curing and environmental conditions, etc. The design should be based on 28 days characteristic strength of concrete unless there is an evidence to justify a higher strength for a particular structure due to age.
5.2.1.1 For concrete of grade M 30 and above, the rate of increase of compressive strength with age shall be based on actual investigations.
5.2.1.2 Where members are subjected to lower direct load during construction, they should be checked for stresses resulting from combination of direct load and bending during construction.
The flexural and splitting tensile strengths shall be obtained in accordance with good practice [6-5A(18)]. When the designer wishes to use an estimate of the tensile strength from the compressive strength, the following formula may be used:
Flexural strength, fcr = 0.7√fck N/mm²
where
fck = characteristic cube compressive strength of concrete, in N/mm ² .
The modulus of elasticity is primarily influenced by the elastic properties of the aggregate and to a lesser extent by the conditions of curing and age of the concrete, the mix proportions and the type of cement. The modulus of elasticity is normally related to the compressive strength of concrete.
5.2.3.1 The modulus of elasticity of concrete can be assumed as follows:
The total shrinkage of concrete depends upon the constituents of concrete, size of the member and environmental conditions. For a given humidity and temperature, the total shrinkage of concrete is most influenced by the total amount of water present in the concrete at the time of mixing and, to a lesser extent, by the cement content.
5.2.4.1 In the absence of test data, the approximate value of the total shrinkage strain for design may be taken as 0.0003 {for more information, see accepted standard [6-5A(19)]}.
Creep of concrete depends, in addition to the factors listed in 5.2.4, on the stress in the concrete, age at loading and the duration of loading. As long as the stress in concrete does not exceed one-third of its characteristic compressive strength, creep may be assumed to be proportional to the stress.
5.2.5.1 In the absence of experimental data and detailed information on the effect of the variables, the ultimate creep strain may be estimated from the following values of creep coefficient (that is, ultimate creep strain/elastic strain at the age of loading); for long span structure, it is advisable to determine actual creep strain, likely to take place:
| Age at Loading | Creep Coefficient |
|---|---|
| 7 days | 2.2 |
| 28 days | 1.6 |
| 1 year | 1.1 |
NOTE — The ultimate creep strain, estimated as described above does not include the elastic strain.
The coefficient of thermal expansion depends on nature of cement, the aggregate, the cement content, the relative humidity and the size of sections.
The value of coefficient of thermal expansion for concrete with different aggregates may be taken as given below:
| Type of Aggregate | Coefficient of Thermal Expansion for Concrete/°C |
|---|---|
| Quartzite | 1.2 to 1.3 × 10⁻⁵ |
| Sandstone | 0.9 to 1.2 × 10⁻⁵ |
| Granite | 0.7 to 0.95 × 10⁻⁵ |
| Basalt | 0.8 to 0.95 × 10⁻⁵ |
| Limestone | 0.6 to 0.9 × 10⁻⁵ |
A durable concrete is one that performs satisfactorily in the working environment during its anticipated exposure conditions during service life. The materials and mix proportions specified and used should be such as to maintain its integrity and, if applicable, to protect embedded metal from corrosion.
7.1.1 One of the main characteristics influencing the durability of concrete is its permeability to the ingress of water, oxygen, carbon dioxide, chloride, sulphate and other potentially deleterious substances. Impermeability is governed by the constituents and workmanship used in making the concrete. With normal-weight aggregates a suitably low permeability is achieved by having an adequate cement content, sufficiently low free water/
cement ratio, by ensuring complete compaction of the concrete, and by adequate curing.
The factors influencing durability include,
a) the environment;
b) the cover to embedded steel;
c) the type and quality of constituent materials;
d) the cement content and water/cement ratio of the concrete;
e) workmanship, to obtain full compaction and efficient curing; and
f) the shape and size of the member.
The degree of exposure anticipated for the concrete during its service life together with other relevant factors relating to mix composition, workmanship, design and detailing should be considered. Maintenance plays an important role in sustained durability of concrete (see also 9.1). The concrete mix to provide adequate durability under these conditions should be chosen taking account of the accuracy of current testing regimes for control and compliance as described in this Section.
The mix proportion shall be selected to ensure the workability of the fresh concrete and when concrete is hardened, it shall have the required strength, durability and surface finish.
8.1.1 The determination of the proportions of cement, aggregates and water to attain the required strengths shall be made as follows:
a) By designing the concrete mix; such concrete shall be called 'Design mix concrete', or
b) By adopting nominal concrete mix; such concrete shall be called ‘Nominal mix concrete’.
Design mix concrete is preferred to nominal mix. If design mix concrete cannot be used for any reason on the work for grades of M 20 or lower, nominal mixes may be used with the permission of Engineer-in-Charge, which, however, is likely to involve a higher cement content.
In specifying a particular grade of concrete, the following information shall be included:
a) Type of mix, that is, design mix concrete or nominal mix concrete;
b) Grade designation;
c) Type of cement;
d) Maximum nominal size of aggregate;
e) Minimum cement content (for design mix concrete);
f) Maximum water-cement ratio;
g) Workability;
h) Mix proportion (for nominal mix concrete);
j) Exposure conditions as per Tables 4 and 5;
k) Maximum temperature of concrete at the time of placing;
m) Method of placing; and
n) Degree of supervision.
8.1.2.1 In appropriate circumstances, the following additional information may be specified:
a) Type of aggregate,
b) Maximum cement content, and
c) Whether an admixture shall or shall not be used and the type of admixture and the condition of use.
8.2.1 As the guarantor of quality of concrete used in the construction, the constructor shall carry out the mix design and the mix so designed (not the method of design) shall be approved by the employer within the limitations of parameters and other stipulations laid down by this standard. If so desired, the employer shall be provided with supporting data including graphs showing strength versus water-cement ratio for range of proportions, complete trial mix proportioning details to substantiate the choice of cement content, fine and coarse aggregate content, water, mineral admixtures, chemical admixtures, etc.
8.2.2 The mix shall be designed to produce the grade of concrete having the required workability and a characteristic strength not less than appropriate values given in Table 2. Proportion/grading of aggregates shall be made by trial in such a way as to make densest possible concrete. The target mean strength of concrete mix should be equal to the characteristic strength plus
1.65 times the standard deviation.
8.2.3 Mix design done earlier not prior to one year may be considered adequate for later work provided there is no change in source and the quality of the materials.
The standard deviation for each grade of concrete shall be calculated, separately.
8.2.4.1 Standard deviation based on test strength of sample
a) Number of test results of samples — The total number of test strength of samples required to constitute an acceptable record for calculation of standard deviation shall be not less than 30. Attempts should be made to obtain the 30 samples, as early as possible, when a mix is used for the first time.
b) In case of significant changes in concrete — When significant changes are made in the production of concrete batches (for example changes in the materials used, mix design, equipment or technical control), the standard deviation value shall be separately calculated for such batches of concrete.
c) Standard deviation to be brought up to date — The calculation of the standard deviation shall be brought up to date after every change of mix design.
Where sufficient test results for a particular grade of concrete are not available, the value of standard deviation given in Table 8 may be assumed for design of mix in the first instance. As soon as the results of samples are available, actual calculated standard deviation shall be used and the mix designed properly. However, when adequate past records for a similar grade exist and justify to the designer a value of standard deviation different from that shown in Table 8, it shall be permissible to use that value.
Nominal mix concrete may be used for concrete of M 20 or lower. The proportions of materials for nominal mix concrete shall be in accordance with Table 9.
8.3.1 The cement content of the mix specified in Table 9 for any nominal mix shall be proportionately increased if the quantity of water in a mix has to be increased to overcome the difficulties of placement and compaction, so that the water-cement ratio as specified is not exceeded.
| (SI No. | Grade of Concrete | Assumed Standard Deviation N/mm² |
| (1) | (2) | (3) |
| i) | M 10 } | 3.5 |
| ii) | M 15 } | |
| iii) | M 20 } | 4.0 |
| M 25 } | ||
| iv) | M 30 } | |
| v) | M 35 | |
| vi) | M 40 | |
| vii) | M 45 } | 5.0 |
| viii) | M 50 | |
| ix) | M 55 | |
| x) | M 60 | |
| NOTES1 The above values correspond to the site control having proper storage of cement; weigh batching of all materials; controlled addition of water; regular checking of all materials, aggregate grading and moisture content; and periodical checking of workability and strength. Where there is deviation from the above, the values given in the above table shall be increased by 1 N/mm² .2 For grades above M 60, the standard deviation shall be established by actual trials based on assumed proportions, before finalizing the mix. | ||
The shape or design details of exposed structures should be such as to promote good drainage of water and to avoid standing pools and rundown of water. Care should also be taken to minimise any cracks that may collect or transmit water. Adequate curing is essential to avoid the harmful effects of early loss of moisture (see 12.5). Member profiles and their intersections with other members shall be designed and detailed in a way to ensure easy flow of concrete and proper compaction during concreting.
Concrete is more vulnerable to deterioration due to chemical or climatic attack when it is in thin sections, in sections under hydrostatic pressure from one side only, in partially immersed sections and at corners and edges of elements. The life of the structure can be lengthened by providing extra cover to steel, by chamfering the corners or by using circular cross-sections or by using surface coatings which prevent or reduce the ingress of water, carbon dioxide or aggressive chemicals.
The general environment to which the concrete will be exposed during its working life is classified into five levels of severity, that is, mild, moderate, severe, very severe and extreme as described in Table 3.
| Sl No. | Environment | Exposure Conditions |
|---|---|---|
| (1) | (2) | (3) |
| i) | Mild | Concrete surfaces protected against weather or aggressive conditions, except those situated in coastal area |
| ii) | Moderate | a) Concrete surfaces sheltered from severe rain or freezing whilst wetb) Concrete exposed to condensation and rainc) Concrete continuously under waterd) Concrete in contact or buried under non-aggressive soil/ground watere) Concrete surfaces sheltered from saturated salt air in coastal area |
| iii) | Severe | a) Concrete surfaces exposed to severe rain, alternate wetting and drying or occasional freezing whilst wet or severe condensationb) Concrete completely immersed in sea waterc) Concrete exposed to coastal environment |
| iv) | Very severe | a) Concrete surfaces exposed to sea water spray, corrosive fumes or severe freezing conditions whilst wetb) Concrete in contact with or buried under aggressive sub-soil/ground water |
| v) | Extreme | a) Surface of members in tidal zoneb) Members in direct contact with liquid/solid aggressive chemicals |
Abrasion of concrete surfaces results from friction, which may cause a grinding action; or by repetitive impact and overloading, which causes local crushing.
Abrasion resistant surfaces primarily involve consideration of surface finishing technique curing regime, aggregate characteristics and cement content. Compressive strength of concrete may also provide a relative indication of resistance.
Specialist literatures may be referred to for durability requirements of concrete surfaces exposed to abrasive action, for example, in case of machinery and metal tyres.
Where freezing and thawing actions under wet conditions exist, enhanced durability can be obtained by the use of suitable air entraining admixtures. When concrete lower than grade M 50 is used under these conditions, the mean total air content by volume of the fresh concrete at the time of delivery into the construction should be:
| Nominal Maximum Size Aggregate mm | Entrained Air Percentage |
|---|---|
| 10 | 7 ± 1 |
| 20 | 5 ± 1 |
| 40 | 4 ± 1 |
Since air entrainment reduces the strength, suitable adjustments may be made in the mix design for achieving required strength.
Table 4 gives recommendations for the type of cement, maximum free water/cement ratio and minimum cement content, which are required at different sulphate concentrations in near-neutral ground water having pH of 6 to 9.
For the very high sulphate concentrations in Class 5 conditions, some form of lining such as polyethylene or polychloroprene sheet; or surface coating based on asphalt, chlorinated rubber, epoxy; or polyurethane materials should also be used to prevent access by the sulphate solution.
7.2.3.1 The protection of the steel in concrete against corrosion depends upon an adequate thickness of good quality concrete.
7.2.3.2 The nominal cover to the reinforcement shall be provided as per 25.4.
The free water-cement ratio is an important factor in governing the durability of concrete and should always be the lowest value. Appropriate values for minimum cement content and the maximum free water-cement ratio are given in Table 5 for different exposure conditions. The minimum cement content and maximum water-cement ratio apply to 20 mm nominal maximum size aggregate. For other sizes of aggregate they should be changed as given in Table 6.
Cement content not including fly ash and ground granulated blast furnace slag in excess of 450 kg/m³ should not be used unless special consideration has been given in design to the increased risk of cracking due to drying shrinkage in thin sections, or to early thermal cracking and to the increased risk of damage due to alkali silica reactions.
7 Where chloride is encountered along with sulphates in soil or ground water, ordinary Portland cement with C₃A content from 5 to 8 percent shall be desirable to be used in concrete, instead of sulphate resisting cement. Alternatively, Portland slag cement conforming to accepted standard [6-5A(21)] having more than 50 percent slag or a blend of ordinary Portland cement and slag may be used.
| Sl No. | Class | Concentration of Sulphates, Expressed as SO₃ | Type of Cement | Dense, Fully Compacted Concrete. Made with 20 mm Nominal Maximum Size Aggregates in Accordance with Accepted Standard [6-5A(12)] | |||
| In Soil | In Ground Water | ||||||
| Total SO₃ | SO₃ in 2:1 Water: Soil Extract | ||||||
| Percent | g/l | g/l | Minimum Cement Content kg/m³ | Maximum Free Water-Cement Ratio | |||
| (1) | (2) | (3) | (4) | (5) | (6) | (7) | (8) |
| i) | 1 | Traces (<0.2) | Less than 1.0 | Less than 0.3 | Ordinary Portland cement or Portland slag cement or Portland pozzolana cement | 280 | 0.55 |
| ii) | 2 | 0.2 to 0.5 | 1.0 to 1.9 | 0.3 to 1.2 | Ordinary Portland cement or Portland slag cement or Portland pozzolana cement | 330 | 0.50 |
| iii) | 3 | ||||||
For concrete to be durable, careful selection of the mix and materials is necessary, so that deleterious constituents do not exceed the limits.
Whenever there is chloride in concrete there is an increased risk of corrosion of embedded metal. The higher the chloride content, or if subsequently exposed to warm moist conditions, the greater the risk of corrosion. All constituents may contain chlorides and concrete may be contaminated by chlorides from the external environment. To minimise the chances of
deterioration of concrete from harmful chemical salts, the levels of such harmful salts in concrete coming from concrete materials, that is, cement, aggregates, water and admixtures, as well as by diffusion from the environment should be limited. The total amount of chloride content (as Cl) in the concrete at the time of placing shall be as given in Table 7.
The total acid soluble chloride content should be calculated from the mix proportions and the measured chloride contents of each of the constituents. Wherever possible, the total chloride content of the concrete should be determined.
Sulphates are present in most cements and in some
Table 5 Minimum Cement Content, Maximum Water-Cement Ratio and Minimum Grade of Concrete for Different Exposures with Normal Weight Aggregates of 20 mm Nominal Maximum Size
(Clauses 5.1.2, 5.1.3, 7.2.4.1 and 8.1.2)
| Sl No. | Exposure | Plain Concrete | Reinforced Concrete | ||||
| Minimum Cement Content kg/m³ | Maximum Free Water-Cement Ratio | Minimum Grade of Concrete | Minimum Cement Content kg/m³ | Maximum Free Water-Cement Ratio | Minimum Grade of Concrete | ||
| (1) | (2) | (3) | (4) | (5) | (6) | (7) | (8) |
| i) | Mild | 220 | 0.60 | ? | 300 | 0.55 | M 20 |
| ii) | Moderate | 240 | 0.60 | M 15 | 300 | 0.50 | M 25 |
| iii) | Severe | 250 | 0.50 | M 20 | 320 | 0.45 | M 30 |
| iv) | Very severe | 260 | 0.45 | M 20 | 340 | 0.45 | M 35 |
The destructive action of aggressive waters on concrete is progressive. The rate of deterioration decreases as the concrete is made stronger and more impermeable, and increases as the salt content of the water increases. Where structures are only partially immersed or are in contact with aggressive soils or waters on one side only, evaporation may cause serious concentrations of salts with subsequent deterioration, even where the original salt content of the soil or water is not high.
NOTE — Guidance regarding requirements for concrete exposed to sulphate attack is given in 7.2.2.4.
At sites where alkali concentrations are high or may become very high, the ground water should be lowered by drainage so that it will not come into direct contact with the concrete.
Additional protection may be obtained by the use of suitable impermeable barriers.
Adequate compaction without segregation should be ensured by providing suitable workability and by employing appropriate placing and compacting equipment and procedures. Full compaction is particularly important in the vicinity of construction and movement joints and of embedded water bars and reinforcement.
Good finishing practices are essential for durable concrete.
Overworking the surface and the addition of water/cement to aid in finishing should be avoided; the resulting laitance will have impaired strength and durability and will be particularly vulnerable to freezing and thawing under wet conditions.
It is essential to use proper and adequate curing techniques to reduce the permeability of the concrete and enhance its durability by extending the hydration of the cement, particularly in its surface zone (see 12.5).
Concrete in sea-water or exposed directly along the sea-coast shall be at least M 20 Grade in the case of plain concrete and M 30 in case of reinforced concrete. The use of slag or pozzolana cement is advantageous under such conditions.
7.2.8.1 Special attention shall be given to the design of the mix to obtain the densest possible concrete; slag, broken brick, soft limestone, soft sandstone, or other porous or weak aggregates shall not be used.
7.2.8.2 As far as possible, preference shall be given to precast members unreinforced, well-cured and hardened, without sharp corners, and having trowel-smooth finished surfaces free from crazing, cracks or other defects; plastering should be avoided.
7.2.8.3 No construction joints shall be allowed within 600 mm below low water-level or within 600 mm of the upper and lower planes of wave action. Where unusually severe conditions or abrasion are anticipated, such parts of the work shall be protected by bituminous or silico-fluoride coatings or stone facing bedded with bitumen.
7.2.8.4 In reinforced concrete structures, care shall be taken to protect the reinforcement from exposure to saline atmosphere during storage, fabrication and use. It may be achieved by treating the surface of reinforcement with cement wash or by suitable methods.
9.1.1 In order that the properties of the completed structure be consistent with the requirements and the assumptions made during the planning and the design, adequate quality assurance measures shall be taken. The construction should result in satisfactory strength, serviceability and long term durability so as to lower the overall life-cycle cost. Quality assurance in construction activity relates to proper design, use of adequate materials and components to be supplied by the producers, proper workmanship in the execution of works by the contractor and ultimately proper care during the use of structure including timely maintenance and repair by the owner. The maintenance plays an important role in sustained durability of concrete.
9.1.2 Quality assurance measures are both technical and organizational. Some common cases should be specified in a general Quality Assurance Plan which shall identify the key elements necessary to provide fitness of the structure and the means by which they are to be provided and measured with the overall purpose to provide confidence that the realized project will work satisfactorily in service fulfilling intended needs. The job of quality control and quality assurance would involve quality audit of both the inputs as well as the outputs. Inputs are in the form of materials for concrete; workmanship in all stages of batching, mixing, transportation, placing, compaction and curing;
| Table 9 Proportions for Nominal Mix Concrete(Clauses 8.3 and 8.3.1) | ||||
| Sl No. | Grade of Concrete | Total Quantity of Dry Aggregates by Mass per 50 kg of Cement, to be Taken as the Sum of the Individual Masses of Fine and Coarse Aggregates kgMax | Proportion of Fine Aggregate to Coarse Aggregate (by Mass) | Quantity of Water per 50 kg of Cement1 |
| (1) | (2) | (3) | (4) | (5) |
| i) | M 5 | 800 | Generally 1:2 | 60 |
| ii) | M 7.5 | 625 | but subject to an upper limit | 45 |
| iii) | M 10 | 480 | 34 | |
| iv) | M 15 | 330 | of 1 : 1(1)/(2) and a lower limit of 1 : 2(1)/(2) | 32 |
| v) | M 20 | 250 | 30 | |
1 The proportion of the fine to coarse aggregates should be adjusted from upper limit to lower limit progressively as the grading of fine aggregates becomes finer and the maximum size of coarse aggregate becomes larger. Graded coarse aggregate shall be used.
Example
For an average grading of fine aggregate {that is, Zone II of Table 4 of the accepted standard [6-5A(12)]}, the proportions shall be 1:1(1)/(2), 1:2 and 1:2(1)/(2) for maximum size of aggregates 10mm, 20mm and 40mm, respectively.
2 Quantity of water required from durability point of view may be less than the value given above.
and the related plant, machinery and equipment; resulting in the output in the form of concrete in place. To ensure proper performance, it is necessary that each step in concreting which will be covered by the next step is inspected as the work proceeds (see also 16).
9.1.3 Each party involved in the realization of a project should establish and implement a Quality Assurance Plan, for its participation in the project. Supplier's and subcontractor's activities shall be covered in the plan. The individual Quality Assurance Plans shall fit into the general Quality Assurance Plan. A Quality Assurance Plan shall define the tasks and responsibilities of all persons involved, adequate control and checking procedures, and the organization and maintaining adequate documentation of the building process and its results. Such documentation should generally include,
a) test reports and manufacturer's certificate for materials, concrete mix design details;
b) pour cards for site organization and clearance for concrete placement;
c) record of site inspection of workmanship, field tests;
d) non-conformance reports, change orders;
e) quality control charts; and
f) statistical analysis.
NOTE — Quality control charts are recommended, wherever the concrete is in continuous production over considerable period.
To avoid confusion and error in batching, consideration should be given to using the smallest practical number of different concrete mixes on any site or in any one plant. In batching concrete, the quantity of both cement and aggregate shall be determined by mass; admixture, if solid, by mass; liquid admixture may however be measured in volume or mass; water shall be weighed or measured by volume in a calibrated tank {see also accepted standard [6-5A(23)]}.
For large and medium project sites, the concrete shall be sourced from ready-mixed concrete plants or from captive on-site or off-site automatic batching and mixing plants. The concrete produced and supplied by ready-mixed concrete plants shall be in accordance with good practices [6-5A(24)]. In case of concrete from captive on-site or off-site automatic batching and mixing plants, similar quality control shall be followed.
9.2.1 The grading of aggregate shall be controlled by obtaining the coarse aggregate in different sizes and blending them in right proportions, the different sizes being stocked in separate stock-piles. The material should be stock-piled for several hours preferably a day before use. The grading of coarse and fine aggregate should be checked as frequently as possible, the frequency for a given job being determined by the Engineer-in-Charge to ensure that the specified grading is maintained.
9.2.2 The accuracy of the measuring equipment shall be within ± 2 percent of the quantity of cement and mineral admixtures being measured and within ± 3 percent of the quantity of aggregate, chemical admixtures and water being measured. In a batching plant, the concrete production equipment shall be calibrated initially at the time of installation or reconditioning of the equipment and subsequently at the following intervals:
a) Mechanical/knife edge: At least once every systems two months
b) Electrical/load cell systems : At least once every three months
9.2.3 All ingredients of concrete shall be used by mass only except water and chemical admixtures, which may be by volume.
9.2.4 Volume batching may be allowed only where weigh-batching is not practical and provided accurate bulk densities of materials to be actually used in concrete have earlier been established. Allowance for bulking shall be made in accordance with accepted standard [6-5A(25)]. The mass volume relationship should be checked as frequently as necessary, the frequency for the given job being determined by Engineer-in-Charge
to ensure that the specified grading is maintained.
9.2.5 It is important to maintain the water-cement ratio constant at its correct value. To this end, determination of moisture contents in both fine and coarse aggregates shall be made as frequently as possible, the frequency for a given job being determined by the Engineer-in-Charge according to weather conditions. The amount of the added water shall be adjusted to compensate for any observed variations in the moisture contents. For the determination of moisture content in the aggregates, accepted standard [6-5A(25)] may be referred to. Where batching plants are used, it is recommended to determine moisture content by moisture probes fitted to the batching plants. To allow for the variation in mass of aggregate due to variation in their moisture content, suitable adjustments in the masses of aggregates shall also be made. In the absence of exact data, only in the case of nominal mixes, the amount of surface water may be estimated from the values given in Table 10.
Concrete shall be mixed in a mechanical mixer {(see also the accepted standard [6-5A(26)]}. It shall be ensured that stationary or central mixers and truck mixers shall comply with the performance criteria of mixing efficiency as per the accepted standard [6-5A(27)]. Mixing efficiency test shall be performed at least once in a year. The mixers shall be fitted with water measuring (metering) devices. The mixing shall be continued until there is a uniform distribution of the materials and the mass is uniform in colour and consistency. If there is segregation after unloading from the mixer, the concrete should be remixed.
9.3.1 As a guidance, the mixing time shall be at least 2 min for conventional free fall (drum) batch type concrete mixers. For other types of more efficient mixers, manufacturer's recommendations shall be followed.
9.3.2 Workability should be checked at frequent intervals {see accepted standard [6-5A(20)]}.
9.3.3 Dosages of retarders, plasticizers and superplasticizers shall be restricted to 0.5, 1.0 and 2.0 percent, respectively by mass of cementitious materials; however, the dosages of polycarboxylate based admixtures shall not exceed 1.0 percent. A higher value of above admixtures may be used, if agreed upon between the manufacturer and the constructor based on performance tests relating to workability, setting time and early age strength.
4.4.1.3 The initial setting time of test block made with the appropriate cement and the water proposed to be used shall not be less than 30 min and shall not differ by ± 30 min from the initial setting time of control test block prepared with the same cement and distilled water. The test blocks shall be prepared and tested in accordance with the good practice [6-5A(15)].
4.4.2 The pH value of water shall be not less than 6.
Sea water shall not be used for mixing or curing of concrete because of presence of harmful salts. Under unavoidable circumstances sea water may be used for mixing or curing in plain concrete with no embedded steel after having given due consideration to possible disadvantages and precautions including use of appropriate cement system.
4.4.4 Water found satisfactory for mixing is also suitable for curing concrete. However, water used for curing should not produce any objectionable stain or unsightly deposit on the concrete surface.
where
Ec = short term static modulus of elasticity, in N/mm ² .
Actual measured values may differ by ± 20 percent from the values obtained from the above expression.
| 0.5 to 1.0 |
| 1.9 to 3.1 |
| 1.2 to 2.5 |
| Supersulphated cement or sulphate resisting Portland cement |
| 310 |
| 0.50 |
| Supersulphated cement or sulphate resisting Portland cement | 330 | 0.50 |
| Portland pozzolana cement or Portland slag cement | 350 | 0.45 |
| iv) | 4 | 1.0 to 2.0 | 3.1 to 5.0 | 2.5 to 5.0 | Supersulphated or sulphate resisting Portland cement | 370 | 0.45 |
| v) | 5 | More than 2.0 | More than 5.0 | More than 5.0 | Sulphate resisting Portland cement or supersulphated cement with protective coatings | 400 | 0.40 |
NOTES
1 Cement content given in this table is irrespective of grades of cement.
2 Use of supersulphated cement is generally restricted where the prevailing temperature is above 40°C.
3 Supersulphated cement gives an acceptable life provided that the concrete is dense and prepared with a water-cement ratio of 0.4 or less, in mineral acids, down to pH 3.5.
4 The cement contents given in col 7 of this table are the minimum recommended. For SO₃ contents near the upper limit of any class, cement contents above these minimum are advised. For the purpose of calculation of SO₃ content (if the test results are in the form of SO₄), the following relation shall be used: SO₃ = 0.833SO₄.
5 For severe conditions, such as thin sections under hydrostatic pressure on one side only and sections partly immersed, considerations should be given to a further reduction of water-cement ratio.
6 Portland slag cement conforming to accepted standard [6-5A(21)] with slag content more than 50 percent exhibits better sulphate resisting properties.
| v) |
| Extreme |
| 280 |
| 0.40 |
| M 25 |
| 360 |
| 0.40 |
| M 40 |
| NOTES |
| 1 Cement content prescribed in this table is irrespective of grades and types of cement and is inclusive of mineral admixtures mentioned in 4.2. The mineral admixtures such as fly ash or ground granulated blast furnace slag shall be taken into account in the concrete composition with respect to the minimum cement content and maximum water-cement ratio not exceeding the limit of fly ash and slag specified in accordance with accepted standards [6-5A(22)] and [6-5A(21)], beyond which these additions, though permitted, shall not be considered for these purposes. |
| 2 Minimum grade for plain concrete under mild exposure condition is not specified. |
| 3 The minimum cement content, maximum free water-cement ratio and minimum grade of concrete are individually related to exposure. |
| Sl No. | Nominal Maximum Aggregate Size | Adjustments to Minimum Cement Contents in Table 5 |
|---|---|---|
| mm | kg/m³ | |
| (1) | (2) | (3) |
| i) | 10 | +40 |
| ii) | 20 | 0 |
| iii) | 40 | -30 |
| Sl No. | Type or Use of Concrete | Maximum Total Acid Soluble Chloride Content Expressed as kg/m3of Concrete |
|---|---|---|
| (1) | (2) | (3) |
| i) | Concrete containing metal and steam cured at elevated temperature and prestressed concrete | 0.4 |
| ii) | Reinforced concrete or plain concrete containing embedded metal | 0.6 |
| iii) | Concrete not containing embedded metal or any material requiring protection from chloride | 3.0 |
aggregates; excessive amounts of water-soluble sulphate from these or other mix constituents can cause expansion and disruption of concrete. To prevent this, the total water-soluble sulphate content of the concrete mix, expressed as SO₃ (where SO₃=0.833 SO₄ ), should not exceed 4 percent by mass of the cement in the mix. The sulphate content should be calculated as the total from the various constituents of the mix.
The 4 percent limit does not apply to concrete made with supersulphated cement complying with accepted standard [6-5A(6)].
Some aggregates containing particular varieties of silica may be susceptible to attack by alkalis ( Na₂O and K₂O ) originating from cement or other sources, producing an expansive reaction which can cause cracking and disruption of concrete. Damage to concrete from this reaction will normally only occur when all the following are present together:
a) A high moisture level, within the concrete;
b) A cement with high alkali content, or another source of alkali; and
c) Aggregate containing an alkali reactive constituent.
Where the service records of particular cement/aggregate combination are well established, and do not include any instances of cracking due to alkali-aggregate reaction, no further precautions should be necessary. When the materials are unfamiliar, precautions should take one or more of the following forms:
a) Use of non-reactive aggregate from alternate sources.
b) Use of low alkali ordinary Portland cement having total alkali content not more than 0.6 percent (as Na₂O equivalent).
Further advantage can be obtained by use of fly ash conforming to accepted standard [6-5A(7)] or granulated blast furnace slag conforming to accepted standard [6-5A(10)] as part replacement of ordinary Portland cement (having total alkali content as Na₂O equivalent not more than 0.6 percent), provided fly ash content is at least 25 percent or slag content is at least 50 percent.
c) Measures to reduce the degree of saturation of the concrete during service such as use of impermeable membranes.
d) Limiting the cement content in the concrete mix and thereby limiting total alkali content in the concrete mix. For more guidance, specialist literatures may be referred.
| Sl No. | Aggregate | Approximate Quantity of Surface Water | |
| Percent by Mass(3) | litre/m³ (4) | ||
| (1) | (2) | ||
| i) | Very wet sand | 7.5 | 120 |
| ii) | Moderately wet sand | 5.0 | 80 |
| iii) | Moist sand | 2.5 | 40 |
| iv) | Moist gravel or crushed rock ¹⁾ | 1.25-2.5 | 20-40 |
9.2.6 No substitutions in materials used on the work or alterations in the established proportions, except as permitted in 9.2.4 and 9.2.5 shall be made without additional tests to show that the quality and strength of concrete are satisfactory.